Unit |
C50 |
CM¢ó |
GM¢óN |
GM¢óK |
GM¢óT |
CM¢óR |
| Density |
g/cm3 |
0.96 |
0.94 |
0.94 |
0.95 |
0.95 |
0.94 |
| Crystalline
melting range |
oC |
135/138 |
135/138 |
135/138 |
135/138 |
135/138 |
135/138 |
| Tensile
stress at break 23oC/120oC |
N/mm2 |
29/3.2 |
22/3.6 |
22/3.6 |
22/3.6 |
22/3.4 |
22/3.3 |
| Tensile stress
at break 23oC/120oC |
N/mm2 |
40/5 |
42/23 |
46/22 |
35/15 |
19/14 |
38/20 |
| Elongation
at break 23oC/120oC |
% |
800/1000 |
600/900 |
600/800 |
400/580 |
360/520 |
500/700 |
| Ball indentation
hardness H132/30 |
N/mm2 |
55 |
42 |
43 |
43 |
47 |
45 |
| Shore
hardness |
- |
D60 |
D65 |
D62 |
D65 |
D65 |
D63 |
| Notched impact
strength 390j/cm |
¡¡ |
no
break |
no
break |
no
break |
no
break |
no
break |
no
break |
| Relative
abrasion loss by"Sand-Slurry"test(CM¢ó=100) |
¡¡ |
325 |
100 |
90 |
80 |
90 |
160 |
| Coefficient of
linear thermal expal expansion |
1/K |
2X10-4 |
2X10-4 |
2X10-4 |
1.9X10-4 |
1.9X10-4 |
1.8X10-4 |
| Dielectric
strength (measured on a 0.2mm thick sheet) |
kV/mm |
90 |
90 |
90 |
- |
- |
- |
| Surface
resistivity(measured on a 1mm thick sheet) |
¦¸ |
>1013 |
>1013 |
>1013 |
>105 |
- |
- |
| Volume
resistivity(measured on a 0.2mm thick sheet) |
¦¸cm |
>1016 |
>1016 |
>1016 |
>103 |
- |
- |
| Min/Max service
temperature |
oC |
-100/+80 |
-269/+90 |
-269/+90 |
-200/+100 |
-269/+90 |
-269/+90 |